GLASS SILICON NEMA GRADE G-7
| BASE MATERIAL | Glass Fibric |
| RESIN | Silicone |
| MILITARY SPECIFICATION | MIL-P-997 |
| MIL-SPEC TYPE | GSG |
| TENSILE STRENGTH | |
| Lengthwise | 23,000 |
| Crosswise | 18,500 |
| COMPREHENSIVE STRENGTH (psi) | |
| Flatwise | 45,000 |
| Edgewise | 14,000 |
| FLEXURAL STRENGTH, MIN — FOR 1/8-IN SPECIMEN (psi) | |
| Lengthwise | 20,000 |
| Crosswise | 18,000 |
| MODULUS OF ELASTICITY, FLEXURAL | |
| Lengthwise | 1,400 m |
| Crosswise | 1,200 m |
| SHEAR STRENGTH (psi) | 17,000 |
| IZOD IMPACT, MIN (ft-lb per in. of notch) | |
| Flatwise | 6.5 |
| Edgewise | 5.5 |
| HARDNESS, ROCKWELL (M-scale) | 100 |
| SPECIFIC GRAVITY | 1.68 |
| COEFFICIENT OF THERMAL EXPANSION (per deg C) | |
| WATER ABSORPTION, MAX IN 25HR (%) | |
| 1/16 in. | .55 |
| 1/2 in. | .2 |
| DIELECTRIC STRENGTH, PERPENDICULAR TO LAMINATION, SHORT-TIME TEST (V-mil) | |
| 1/16 in. | 400 |
| 1/8 in. | 350 |
| DISSIPATION FACTOR, MAX 1 MC, ASTM D-150, Condition A | .003 |
| DIELECTRIC CONSTANT, MAX 1 MC, ASTM D-150, Condition A | 4.2 |
| INSULATION RESISTANCE, 96 HR, 90 PERCENT RH, 95 (megohms) | 2500 |
| BONDING STRENGTH, MIN (lb) | 650 |
| THERMAL CONDUCTIVITY (cal-cm/sec-sq cm-deg C) | 7 X 10-4 |
| MAX. OPERATING TEMP. °F. | 465 |
Machine Design, June 16, 1966